Propriedades do aço En24 BS970 817M40 En24T material equivalente, revenido, resistência e dureza

Properties of steel En24 BS970 817M40 En24T equivalent material, tempering, strength and hardness

Steel Material En24 BS970 817M40 En24T

Properties of En24 Steel BS970 817M40 (En24T Material)

The following tables summarize BS970 817M40 (Material En24T), En24 steel properties and specifications including chemical composition, mechanical properties, hardness, heat treatment, etc.

Chemical composition

The chemical composition of EN24 steel (En24T steel) and BS970 817M40 is listed in the following table.

Chemical Composition (Casting Analysis), %
Country (Region) Standard Steel Grade W Yes Mn P, ≤ S, ≤ Cr No Mo
Great Britain BS 970-1955 En24 (En24T) 0.35-0.45 0.10-0.35 0.45-0.70 0.050 0.05 0.90-1.40 1.3-1.8 0.20-0.35
BS 970-1991 817M40 0.36-0.44 0.10-0.40 0.45-0.70 0.035 0.04 1h00-1h40 1.3-1.7 0.20-0.35

Mechanical properties

The mechanical properties of En24 (En24T) and 817M40 steels are listed in the following tables, including yield strength (yield stress), ultimate tensile strength, shear strength, modulus of elasticity, modulus of elasticity, etc.

Grades:

  • 1 MPa = 1 N/mm2
  • 1 GPa = 1kN/mm2
Reference symbols for tensile strength bands
Symbol Tensile strength, MPa (ksi)
P 550-700 (80-100)
P 625-775 (90-112)
R 700-850 (100-123)
s 775-925 (110-134)
T 850-1000 (123-145)
you 925-1075 (134-156)
V 1000-1150 (145-167)
W 1075-1225 (156-177)
X 1150-1300 (167-188)
s 1225-1375 (177-199)
Z ≥ 1550 (225)
En24T, En24 Mechanical Properties
Standard Steel Hardened and tempered condition Limiting the decision section, in (mm) Tensile strength, tons/in2 (Mpa) [ksi]≥ Yield stress, tons/in2 (Mpa) [ksi]≥ Elongation, %, ≥ Izod impact, ft lb, ≥ Brinell Hardness, HB
BS970-1955 En24 s 6 (152) 50 (772) [112] 38 (587) [85] 20 40 223-277
T 6 (152) 55 (850) [123] 44 (680) [98] 18 40 248-302
you 4 (101) 60 (926) [134] 48 (741) [107] 17 35 269-321
V 2.5 (63.5) 65 (104) [145] 52 (803) [116] 16 35 293-341
W 1.125 (28.5) 70 (1081) [157] 58 (895) [130] 15 30 311-375
X 1.125 (28.5) 75 (1158) [168] 63 (973) [141] 14 25 341-388
s 1.125 (28.5) 80 (1235) [179] 68 (1050) [152] 14 22 363-415
Z 1.125 (28.5) 100 (1544) [224] 85 (1313) [190] 8 8 ≥ 444
Mechanical Properties of BS970 817M40 Steel
Standard Steel Tensile strength, Mpa (ksi), ≥ Yield strength, Mpa (ksi), ≥ 0.2% proof strength Elongation after fracture, 5.65 √S0 , ≥ Impact, Izod (Charpy V-notch impac) in J, ≥ Hardness, HB Diameter between planes or thickness